Grade, Class, Section Thickness Yield Strength, min Tensile Strength, min
Standard Steel UNS Heat Elongation,
Type, Symbol N/mm2 or N/mm2 or Other
Designation Number Number Treatment t, mm t, in. ksi ksi min, %
or Name MPa MPa
≤ 16 --- 185 ---
ISO 630:1995 E 185 --- --- AR 300-540 --- 18 ---
16 < t ≤ 40 --- 175 ---
ASTM A 283/A 283M-03 A --- --- --- --- --- 165 24 310-415 45-60 30 ---
<3 --- 185 --- 310-540 --- --- ---
3 ≤ t ≤ 16 --- 185 --- 290-510 --- 16 ---
EN 10025:1993 S185 1.0035 --- HR
16 < t ≤ 40 --- 175 --- 290-510 --- --- ---
40 < t ≤ 100 --- --- --- 290-510 --- --- ---
≤ 16 --- 205 --- 21
JIS G 3101:1995 SS330 --- --- HR 16 < t ≤ 40 --- 195 --- 330-430 --- 26 ---
> 40 --- 175 --- 28
0.65 ≤ t < 1.6 0.025 ≤ t < 0.064 21
ASTM A 1011/A 1011M-03 30 [205] --- K02502 HR 1.6 ≤ t < 2.5 0.064 ≤ t < 0.097 205 30 340 49 24 ---
2.5 ≤ t < 6.0 0.097 ≤ t < 0.230 25