You are on page 1of 2

Electrical Properties of Poly Ether Aryl Ketone

1) Sample: PEAK with 1% MgO


Thickness of specimen:
Pressure applied: 5N/mm2

Temp(0 C) 90 80 70 60 50 40 30
Tan 10-3 66 64 63 61 63.5 60 68

7.525 8.597 10.251 10.812 10.497 10.421 10.570


Resistance( ) 3.05 3.15 3.72 4.4 5.25 5.3 3.9
1014
Specific Resistively( 21.03 21.72 25.65 30.34 36.20 36.55 26.89
cm) 1015

2) Sample: PEAK with 2% MgO


Thickness of specimen:
Pressure applied: 5N/mm2

Temp(0 C) 90 80 70 60 50 40 30
Tan 10-4 788 801 795 799 775 777 795
7.105 7.104 7.088 7.060 7.061 7.053 7.055
Resistance( ) 2.13 2.56 2.65 2.80 3.34 3.72 3.95
1014
Specific Resistively( 10.6 17.6 18.2 19.31 23.03 25.65 27.24
cm) 1015

3) Sample: PEAK with 3% MgO


Thickness of specimen:
Pressure applied: 5N/mm2

Temp(0 C) 90 80 70 60 50 40 30
Tan 10-3 60 77 72 72 68 68 77
7.756 5.547 6.343 5.850 6.385 6.480 5.504
Resistance( ) 1.56 2.78 3.5 4.5 4 6.8 7.3
1014
Specific Resistively( 10.7 19.17 24.13 31.03 27.58 46.89 50.34
cm) 1015
4) Sample: PEAK with 4% MgO
Thickness of specimen:
Pressure applied: 5N/mm2

Temp(0 C) 90 80 70 60 50 40 30
Tan 10-4 68.7 61.4 600 500 738 740 7770
2.510 2.499 6.740 6.750 6.782 6.841 5.816
Resistance( ) 120 141 2.44 2.00 2.80 2.68 2.59
1014
Specific Resistively( 82.75 97.2 1.758 1.379 1.931 1.848 1.786
cm) 1016

5) Sample: PEAK with 5% MgO


Thickness of specimen:
Pressure applied: 5N/mm2

Temp(0 C) 90 80 70 60 50 40 30
Tan (10-4 ) 66.0 66.0 755 756 749 796 771

2.309 2.313 6.562 6.550 6.540 7.099 7.200


Resistance( ) 1.23 1.41 0.0091 0.0258 0.0265 0.024 0.040
106

Specific 7.809 8.952 0.06 0.1691 0.1737 0.1573 0.2622


Resistively( c
m) 1017